Tungsten Ore Processing Flowchart
Below is a generalized flowchart for separating tungsten ore (applicable to both wolframite and scheelite), with variations noted based on mineral type:
1. Comminution
Crushing: Jaw/cone crushers reduce ore to ≤10 mm.
Grinding: Ball mills grind ore to 50–150 µm to liberate tungsten minerals.
2. Pre-Concentration
Screening/Jigging: Remove coarse gangue early (e.g., jigs for gravity pre-concentration).
3. Primary Concentration
Gravity Separation:
Shaking tables, spirals chutes, or centrifugal concentrators exploit high density of tungsten minerals.
Produces a rough concentrate (20–50% WO₃).

4. Secondary Separation
For Wolframite (Fe/MnWO₄):
Magnetic Separation: Use low-intensity magnets to separate wolframite (weakly magnetic) from non-magnetic gangue.
For Scheelite (CaWO₄):
Froth Flotation:
Collectors: Fatty acids (e.g., oleic acid).
Depressants: Sodium silicate for silica/calcite suppression.
Removes sulfides (if present) first, then floats scheelite.

5. Cleaning and Scavenging
Multi-Stage Processing:
Re-process middlings/tailings to improve recovery.
Final concentrate: 60–70% WO₃.